FCS 1.2316 Tool Steel
- Fucheng steel
- China
- 1 Month
- 2000 Tons/Month
1.2316 TOOL STEEL
| Brand | FCS |
| Smelting and Manufacture Method: | LF+VD+Forged |
| Delivery Condition: | Annealed |
| Delivery hardness: | ≤250 HBS |
| UT Test Standard: | Sep 1921-84 Class3 D/d,E/e |


1.2316 STEEL GRADE COMPARISON AND CHEMICAL COMPOSITION COMPARISON
| Standard/Steel Grade | Chemical Composition(%) | |||||||
| C | Si | Mn | Cr | Mo | Ni | |||
| DIN/W-Nr. | X36CrMo17/1.2316 | 0.33~0.43 | ≤1.00 | ≤1.00 | 15.0~17.0 | 1.00~1.30 | ≤1.00 | |
| GB | 3Cr17NiMo | 0.28~0.35 | ≤0.80 | ≤1.00 | 16.0~18.0 | 0.75~1.25 | 0.6~1.00 | |
APPLICATION
1.2316 steel is a highly corrosion-resistant plastic mold steel, mainly used in the fields of plastic injection molds and corrosive plastic processing. In the production of plastic products such as automotive components and electronic casings, it can effectively resist the erosion of acidic gases. 1.2316 steel is particularly suitable for processing chemically aggressive materials such as PVC and halogenated plastics, and performs well in the chemical container and packaging industry.
1.2316 steel is also widely used in high-precision surface requirement molds and hardware tool manufacturing. Its excellent polishing performance makes it an ideal choice for transparent products and medical device molds. In the field of hardware, 1.2316 steel is commonly used to manufacture tools such as wire drawing dies and bolt dies, and its wear resistance is outstanding under heavy load conditions.
1.2316 Steel Characteristics
1.2316 steel is a mold steel with high hardness, wear resistance, and corrosion resistance. The following is a detailed introduction to its functions:
Good corrosion resistance: Due to the high proportion of chromium and molybdenum elements, 1.2316 steel has excellent corrosion resistance and can resist the erosion of most chemicals and corrosive media, thereby extending its service life.
High hardness: Through heat treatment, 1.2316 steel can achieve a high hardness of 30-36HRC, which allows it to withstand a large amount of wear and impact.
Good cutting performance: 1.2316 steel has good cutting performance and can be processed and shaped through various cutting methods, making it an ideal choice for tools such as manufacturing molds, plastic molds, and injection molds.
Good thermal stability: 1.2316 steel has good thermal stability and can maintain its performance in high temperature environments, making it suitable for applications that require working under high temperature conditions, such as injection molds.
Good wear resistance: 1.2316 steel has good wear resistance due to its high proportion of molybdenum element.
In addition, 1.2316 mold steel is also used in plastic molds that require polishing requirements, such as cosmetics molds and stationery molds, due to its excellent polishing performance after pre hardening treatment. At the same time, the steel material also has advantages such as uniform material hardness, superior polishing performance, very high surface accuracy after polishing, and low impurity content.
Heat Treatment
Pre-hardened as supplied – no further heat treatment needed for general use.
Soft Annealing
760–800 °C, hold 4–5 h
Furnace cool at 10–20 °C/h down to ~650 °C
Finish in air, max. 230 HB
Hardening
1030–1050 °C
Soak 15–30 min at target temperature
Quench in water or oil
Resulting hardness: 49 HRC
Tempering
Slow heat to tempering temperature right after hardening
Minimum furnace time: 1 h per 20 mm part thickness